2012年7月23日星期一

How to Activate Molecular Sieves


                                         Molecular  Sieve
Chemists frequently use drying agents to remove water or other contaminants from solvents. Molecular sieve are one of the most effective drying agents. They consist of aluminum, silicon, oxygen and other atoms arranged in a three-dimensional network with open channels; the size of the channels varies depending on the exact ratio of aluminum and silicon. Manufacturers designate the most common channel sizes as 3A, 4A, 5A or 10A, where the number represents the approximate size of the channels in angstroms. Before a scientist can use molecular sieves as a drying agent, she must “activate” them by removing all traces of water and other volatile compounds. Normally, this involves heating the sieves to 300 to 320 degrees Celsius for about 15 hours.

Instructions

1 Place the molecular sieves in a large, heat-resistant beaker or ceramic bowl. Use the largest beaker or bowl that will fit inside the laboratory-grade oven.
2 Place the beaker or bowl inside the oven.
3 Heat the molecular sieves at 300 to 320 degrees Celsius for at least 15 hours. Heating for longer periods is unnecessary, but will not damage the molecular sieves.
4 Remove the molecular sieves from the oven using heat-resistant gloves. If possible, place the molecular sieves in a desiccator to cool. Otherwise, allow the beaker to cool in the open air until it’s warm to the touch, and then transfer the molecular sieves to an airtight container and cap tightly.

Tips & Warnings

The dust from molecular sieves can irritate the upper respiratory tract. Use a dust mask when handling molecular sieves.
You can visit the website http://www.chinasiliconesealants.com/molecular-sieve/  for more helpful information about Molecular Sieves.